Introduction

Abrasive blast cleaned and power tool cleaned steel surfaces are routinely checked to verify the specified surface profile has been achieved. Industry standards such as ASTM D4417, Standard Test Methods for Field Measurement of Surface Profile of Blast Cleaned Steel[1], NACE International SP0287, Standard Practice for Field Measurement of Surface Profile of Abrasive Blast-Cleaned Steel Surfaces Using Replica Tape, and SSPC: The Society for Protective Coatings PA 17, Procedure for Determining Conformance to Steel Profile/Surface Roughness/Peak Count Requirements describe the procedures for performing these measurements, as well as the recommended frequency of measurements and acceptability of the values. However, the standards assume smooth steel was prepared; little is written about measurement of surface profile on rough or irregular surfaces such as pitted steel[2], weathering steel, or cast iron surfaces. This brief article describes a few methods that may be considered for measuring surface profile on these types of irregular surfaces.
Background
Many steel structures that have been in service for relatively long periods of time may have irregular rough surfaces due to corrosion. Often this results in steel thickness loss (section loss), and may even require modification or replacement. But when it is determined that not enough metal loss has occurred to warrant repairs to the steel substrate, the applicator is faced with complying with contract requirements for cleanliness and profile generation on surfaces that have a roughness that often exceeds the surface profile requirements of the contract. 
Measuring surface profile on rough or pitted surfaces can often lead to false high readings, since the measurements are indicative of the depth of the pits or the inherent roughness of the steel versus the surface profile generated by the abrasive or impact-type power tool itself. This begs the question, “how do you verify the surface profile on these types of surfaces with any degree of accuracy?” There are a few alternatives that can be considered; however, they should be discussed, and an approach negotiated during the preconstruction meeting rather than during in-process measurement, when possible.
Alternative Methods


A third option is to measure the surface profile on a companion piece of steel such as a test plate that is abrasive blast cleaned with the same abrasive and pressure being used on the rough steel. This procedure has been accepted in the nuclear power industry for many years when painting cast iron motor housings.
Lastly, the abrasive manufacturer can be consulted regarding the typical surface profile values produced by the type and size abrasive being used. Some abrasive manufacturers can provide a Certificate of Conformance that states the measured range for a given lot under laboratory conditions. Note that surface hardness greatly influences surface profile depth, so the abrasive manufacturer’s data may be misleading.
Conclusion
The important point to remember is that when the surface is rough or irregular, one or more of these methods can be used to more accurately determine the surface profile depth. Further, rough surfaces may require the application of a thicker coat, or additional coating layers to help ensure corrosion protection. The coating manufacturer should be engaged when making these decisions.
[1] According to SSPC-SP 11 and SP 15, verification of minimum 1-mil surface profile created by power tools can only be measured using Method B (depth micrometer) described in the ASTM D4417 standard.
[2] SSPC-PA 17-2012 addresses measurement of surface profile on pitted steel in Appendix C (Section C2.5.3)
[3] ASTM D4417 instructs the operator to report the maximum of the ten measurements; however, this is not recommended on rough/pitted surfaces. The standard does allow averaging of the readings.